Production and Investigation of Natural Zeolite-TiO2/CuO Nanoparticles Composite

Document Type : Research Paper

Authors

Faculty of Materials and Metallurgical Engineering, Semnan University, Semnan, Iran.

Abstract

With the progress of various industries, the ever-increasing production of polluting wastewater has faced mankind with the concern of preserving the environment and providing clean water. The simultaneous use of adsorbents such as natural zeolite and nanophotocatalysts is one of the attractive methods. By doing this, while eliminating the limitations of each, synergy in properties occurs and the performance of pollution removal is improved. In this article, TiO2/CuO nanocomposite was deposited on natural zeolite particles. The produced samples were evaluated and compared with different analyses. The results showed that the presence of the TiO2-7.5% CuO (TC) nanoparticles has improved the ability to absorb UV light despite reducing the specific surface area. The performance of the zeolite-TC combination on the removal of methyl orange (MeO) showed acceptable results. The zeolite sample containing 15%TC with a specific surface area of 29 m2/g and band gap of 3.08 eV removed 93% of MeO dye after 120 min.

Keywords

Main Subjects


Production and Investigation of Natural Zeolite-TiO2/CuO Nanoparticles Composite

  1. Koohestani * , M. Hassanabadi

Faculty of Materials and Metallurgical Engineering, Semnan University, Semnan, Iran

 

KEYWORDS

 

ABSTRACT

Natural zeolite;

TiO2/CuO;

Zeolite/TiO2/CuO;

Industrial waste water;

Nanocomposite.

With the progress of various industries, the ever-increasing production of polluting wastewater has faced mankind with the concern of preserving the environment and providing clean water. The simultaneous use of adsorbents such as natural zeolite and nanophotocatalysts is one of the attractive methods. By doing this, while eliminating the limitations of each, synergy in properties occurs and the performance of pollution removal is improved. In this article, TiO2/CuO nanocomposite was deposited on natural zeolite particles. The produced samples were evaluated and compared with different analyses. The results showed that the presence of the TiO2-7.5% CuO (TC) nanoparticles has improved the ability to absorb UV light despite reducing the specific surface area. The performance of the zeolite-TC combination on the removal of methyl orange (MeO) showed acceptable results. The zeolite sample containing 15%TC with a specific surface area of 29 m2/g and band gap of 3.08 eV removed 93% of MeO dye after 120 min.

 

1.     Introduction

Today, with the rapid development of the industry, large amounts of waste containing various pollutants are produced in many industries. These pollutions severely endanger the environment and the lives of living organisms. Therefore, considering the reduction of water in the world, it is very significant to treat polluted water and return it to the consumption cycle [1, 2].

One of the conventional methods is the use of mineral absorbents. One of these adsorbents is zeolite, which has received a lot of attention. Zeolite is a combination of alumina-silica with a high specific surface area and small pores [3, 4]. The characteristic of ion exchange in zeolite, followed by its high absorption characteristic, has led to its use in the removal of different water pollutants. In addition, zeolite has many applications in agriculture, medicine, and other industries. Zeolite has been used and studied in two natural and artificial forms. Among these unique properties, the use of zeolite is associated with problems. One of the problems of zeolite is the reduction of its absorption capacity due to its saturation with pollutants, therefore it is necessary to recycle them. On the other hand, the efficiency of absorption and removal of pollutants by zeolite needs to be improved to reach the optimal value. There are ways to solve these problems, each of which has specific conditions. One of the useful methods is the use of photocatalysts and their deposition on the surface of zeolite particles [5, 6].

The most widely used photocatalysts are Pt-TiO2, SnO2, NiS-TiO2, and ZnO [7, 8]. Titanium dioxide (TiO2) has attracted a lot of attention due to its unique properties such as cheapness, non-toxicity, optical and chemical stability, etc. One of the drawbacks of using photocatalysts is the high rate of electron-hole recombination in them. This problem limits their application as photocatalysts. In fact, by reducing the recombination rate, the efficiency of the photocatalyst can be improved. In these conditions, making a composite of TiO2 with other semiconductors and thus transferring charge carriers between them can be effective [8, 9]. The presence of copper oxide (CuO) with a band gap of 1.2 eV together with TiO2 with a band gap of about 3.2 eV, in addition to reducing the recombination rate of charge carriers, causes a decrease in the band gap of the composite and a shift of the absorption edge towards visible light [10-13].

The composition of absorbers such as zeolite with photocatalysts improves absorption and condensation properties by creating a synergistic effect. Zeolite as a support material can reduce hole-electron recombination by trapping the photo-induced electrons in the photocatalyst [5, 14]. So far, there has been no research on the deposition of TiO2/CuO nanoparticles on natural zeolite and investigating the performance of the resulting composition. Therefore, in this research, first, the surface of zeolite particles is covered with TiO2/CuO nanoparticles and then the effect of this action on the performance of zeolite is studied with different analyses.

2.     Methodology

For the production of zeolite/TiO2/CuO nanocomposite, natural zeolite prepared from the After mine located in Bakhtar, Semnan province, Iran, with the chemical composition listed in Table 1, was used. Si/Al ratio for zeolite is equal to 5.35, which indicates that the main mineral of zeolite is clinoptilolite [5].

Table 1. Chemical composition of natural zeolite used

compound

SiO2

Al2O3

CaO

MgO

wt%

77.20

12.80

1.96

0.60

compound

K2O

TiO2

Fe2O3

Na2O

wt%

2.55

0.18

0.75

3.60

2.1. Synthesis of Zeolite-TiO2/CuO composite:

Based on previous research [12, 15, 16], the zeolite/TiO2/CuO synthesis process was carried out as follows:

Solution A: First, 85 ml of deionized water, 6 ml of HCl, and 6 ml of 2-propanol were mixed by a stirrer. Then 5 ml of titanium isopropoxide was added drop by drop to the solution. The temperature of the solution slowly reached 60°C in a water bath within 2 h.

Solution B: First, 0.4 g of CuSO4.5H2O was poured into 100 ml of deionized water and stirred for 20 min. Then, 30 ml of 0.05M NaOH was added drop by drop to the solution. After stirring for 30 min, a dark blue solution was obtained, to which 30 ml of 0.05 M ascorbic acid was droply added.

Based on the results of previous works [12], the combination of TiO2-7.5%CuO had the best efficiency. Therefore, solution B was mixed with solution A to synthesize a 7.5%CuO compound. Coarse zeolite particles were crushed by a ball mill for 12 h until particles <100 μm were obtained. Then the resulting powder was washed three times with ethanol and deionized water and finally dried. A certain amount of zeolite powder was added to produce composites containing 5, 10, 15, and 20% TiO2/7.5%CuO with the abbreviation Z5TC, Z10TC, Z15TC, and Z20TC respectively. After stirring for 1 h, the solution was kept overnight at room temperature. Then the precipitation obtained was filtered, dried for 1 h at 80°C, and calcined at 450 °C for 2 h.

2.2. Characterization:

The phases in the produced samples were detected with an X-ray diffractometer (XRD, Bruker D8, Germany) with monochromated Cu-Kα radiation (λ=1.54056 Å). The morphology of the particles was studied with a scanning electron microscope (SEM, XL 30-Philips, Netherlands).

To determine the molecular structure and functional groups on the surface of the particles, infrared spectroscopic analysis (FTIR) was used in the frequency range of 400-14000 cm by ABB-Bomem MB-100 device. The specific surface area of the produced samples was investigated with a BET surface analyzer (Belsorp mini II; Bel, Japan). The band gap value (Eg, eV) of the samples was measured by a UV spectrophotometer at room temperature and was obtained from the starting wavelength (λg, nm) using the following formula [15]:

 

(1)

To evaluate the photocatalytic activity of the samples, the removal of methyl orange (MeO) was performed. 1 g/l sample was added to 50 ml of methyl orange solution (with an initial concentration of 5 ppm and pH=6) at room temperature. Before the start of UV light irradiation (by two 6W lamps-Philips, China), the solution was stirred for 60 min to reach absorption-desorption equilibrium in darkness. The distance of the lamps from the surface of the MeO solution was kept at 10 cm. After 120 min, changes in MeO concentration were determined by a UV-vis spectrophotometer.

3.     Results and Discussion

Figure 1 shows the X-ray diffraction pattern of natural zeolite and Z-15TC composite. According to the peaks of pattern Figure 1a, the zeolite sample is completely crystalline. Investigating its peaks shows the structures of clinoptilolite, aluminum oxide, quartz, and aluminum silicate. The zeolite phases are consistent with the results in Table 1.

In Figure 2b, the pattern of the Z-15TC sample, in addition to various peaks of zeolite-forming compounds, anatase, and CuO peaks are also observed. In the sample synthesis conditions, the main phase of TiO2 was anatase. Rutile peaks have not been detected, which could be due to the detection power of the XRD device, which cannot find phases with small amounts. Another reason is the presence of zeolite, which causes the phase transformation of anatase to rutile to be delayed. This behavior has also been reported in similar studies [15]. The diffraction peaks of the CuO phase are related to the monoclinic crystal structure formed at 450°C [12].

 

 

Fig. 1. XRD patterns of a) natural zeolite and
 b) Z-15TC composite

SEM images of the morphology of natural zeolite samples and Z-15TC composite are presented in Figure 2. Zeolite particles with a non-uniform shape and an approximate size of 0.5-4 µm are observed. After the deposition of TiO2 and CuO nanoparticles on natural zeolite, there is no change in the shape of zeolite particles. Of course, nanoparticles have caused agglomeration to some extent by creating bonds and joins between zeolite particles and creating larger bulks. On the other hand, it has been proven that the addition of nanoparticles to zeolite reduces the pore size of zeolite and thus increases the active sites in the catalyst [15, 16].

In Figure 3, the infrared spectrum shows the type of surface and molecular bonds of the Z-15TC sample. In the range of 400-800 cm-1, the peaks related to the stretching vibrations of the metal-oxygen bond (Ti-O, Cu-O, etc.) and compounds found in natural zeolite have appeared [17, 18]. The peak at 1060 cm-1 is related to vibrations of the Al-O bond and Si-O-Si asymmetric stretching [19]. The peak observed in the range of 1629 cm-1 to 3624 cm-1 indicates the stretching vibration of the H-O-H bond and the stretching vibrations of the hydroxyl O-H bond, respectively [19, 20].

 

Fig. 2. SEM Images of a) natural zeolite and
b) Z-15TC composite

 

Fig. 3. FTIR spectrum of zeolite containing
15% TiO2/7.5%CuO

The specific surface of catalysts and absorbent materials is one of their most important features. Table 2 illustrates the specific surface of different produced samples by the BET method. Natural zeolite has a higher specific surface and by depositing nanoparticles on it, the specific surface decreases [15, 16]. It can be seen here that with the increase in the number of deposited nanoparticles, due to the filling of the surface pores of the zeolite, the specific surface area of the sample decreases. Of course, it was also shown in the SEM images that the deposition of nanoparticles on the zeolite particles caused agglomeration and coarsening of the particles. In research, it was shown that depositing ZnO nanoparticles on the surface of zeolite particles causes the specific surface area to decrease from 52 m2/g to 24 m2/g [21].

Table 2. Specific surface area and absorption
properties of different samples

Sample

specific surface area, m2/g

Absorption edge wavelength, nm

Band gap, eV

Zeolite

35

-

-

Z-5TC

34

370

3.35

Z-10TC

32

384

3.23

Z-15TC

29

403

3.08

Z-20TC

28

418

2.97

 

Fig. 4. Diffuse UV–vis absorbance spectra
 of various samples

One of the most important factors in the evaluation of photocatalytic performance is the evaluation of their optical properties. Figure 4 shows the UV absorption spectrum of different samples. In Table 2, the wavelength of the absorption edge and the value of the band gap of each sample extracted from Figure 4 are shown. Pure zeolite showed no absorption. Pure zeolite showed no absorption. But with the addition of TC nanoparticles, the absorption edge of the sample has a red shift and has been transferred to longer wavelength rays. Finally, the absorption edge of the sample containing 20% TC occurred at 418 nm. As the value of TC increases, the energy of the band gap has decreased. So that the energy of the band gap in the Z20TC sample is about 2.97 eV. The band gap reduction is due to the presence of TiO2 nanoparticles with a band gap of 2.95 eV [12] and CuO nanoparticles with a band gap of 1.37 eV [22]. The band gap of TiO2/7.5% CuO nanoparticles in the absence of zeolite is reported to be 2.53 eV [12]. Therefore, the presence of more nanoparticles on the surface of zeolite particles reduces the band gap.

The removal efficiency of MeO dye by different samples under UV light irradiation is shown in Figure 5. Zeolite has low efficiency due to a lack of photocatalytic properties. The presence of nanoparticles has improved the efficiency because, in addition to the absorption properties of zeolite, the photocatalytic properties of nanoparticles also play an important role. Due to differences in particle surface charge, specific surface area, and band gap energy, the ability of samples to remove MeO varies. The highest efficiency corresponds to the sample Z-15TC (93%).

 

Fig. 5. MeO removal efficiency by different samples
 (time: 120 min, pH=5)

The incorporation of CuO and TiO2 into zeolite particles has a significant effect on light absorption. The increased absorption of the samples in the visible light region is due to the formation of a p-n junction between the p-type CuO semiconductor and the n-type TiO2 semiconductor. In the pure state, the conduction band edge and valence band edge of TiO2 are higher than CuO, and the fermi level of CuO is lower than TiO2. By combining, the fermi level of CuO moves up and the fermi level of TiO2 moves down [10, 11, 23]. Under visible light irradiation, both CuO and TiO2 can be excited to produce electron-hole pairs. Of course, at higher amounts of nanoparticles, because a larger surface area is covered by the zeolite particles, dye absorption is relatively reduced.

4.     Conclusions

In this article, TiO2/CuO nanoparticles were deposited on particles of natural zeolite to simultaneously use the surface adsorption ability of the zeolite and photocatalytic properties of nanoparticles. Deposition of nanoparticles on zeolite, despite the reduction of the specific surface area, causes the reduction of the energy of the band gap. The performance of the samples in the degradation of methyl orange under UV light showed that adding the optimal amount of TiO2/7.5%CuO nanoparticles on the zeolite particles had the best photocatalytic performance. The improvement of photocatalytic efficiency is due to the effective separation of electrons and holes photo-induced in nanoparticles. The p-n junction in TiO2/CuO-zeolite is a strong reason for the enhanced photocatalytic activities.

Conflicts of Interest

No potential conflict of interest was reported by the authors.

References

[1]   Artiola, J., 2019. Industrial waste and municipal solid waste treatment and disposal, in Environmental and pollution science. Elsevie,. pp. 377-391.

[2]   Ambaye, T., Vaccari, M., van Hullebusch, E. D., Amrane, A., & Rtimi, S., 2021. Mechanisms and adsorption capacities of biochar for the removal of organic and inorganic pollutants from industrial wastewater. International Journal of Environmental Science and Technology, 18(10), pp. 3273-3294.

[3]   Wang, S. and Y. Peng, 2010. Natural zeolites as effective adsorbents in water and wastewater treatment. Chemical engineering journal, 156(1), pp. 11-24.

[4]   Metes, A., Kovac̆ević, D., Vujević, D., & Papić, S., 2004. The role of zeolites in wastewater treatment of printing inks. Water Research, 38 (14-15), pp. 3373-3381.

[5]   Korkuna, O., Leboda, R., Skubiszewska-Zie, B. J., Vrublevs’Ka, T., Gun’Ko, V. M., & Ryczkowski, J., 2006. Structural and physicochemical properties of natural zeolites: clinoptilolite and mordenite. Microporous and mesoporous materials, 87(3), pp. 243-254.

[6]   Cui, T., Liu, Z., Zheng, X., Liu, Z., Li, Y., Li, W., Wang, B., Guo, K. and Han, J., 2014. Zeolite-based CuO nanotubes catalysts: investigating the characterization, mechanism, and decolouration process of methylene blue. Journal of nanoparticle research, 16(9), pp. 1-11.

[7]   Sikhwivhilu, L.M., S. Sinha Ray, and N.J. Coville, 2009. Influence of bases on hydrothermal synthesis of titanate nanostructures. Applied Physics A, 94(4), pp. 963-973.

[8]   Liu, Z., Liu, Z., Zheng, X., Liu, Z., Li, Y., Li, W., Wang, B., Guo, K. and Han, J., 2014. Photocatalyst from one-dimensional TiO2 nanowires/synthetic zeolite composites. Materials Express, 4(6), pp. 465-474.

[9]   Koohestani, H. and S.K. Sadrnezhaad, 2016. Improvement in TiO2 photocatalytic performance by ZrO2 nanocompositing and immobilizing. Desalination and Water Treatment, 57(58), pp. 28450-28459.

[10] Subha, P., L. Vikas, and M. Jayaraj, 2018. Solution-processed CuO/TiO2 heterojunction for enhanced room temperature ethanol sensing applications. Physica Scripta, 93(5), p. 055001.

[11] Sawicka-Chudy, P., Sibiński, M., Wisz, G., Rybak-Wilusz, E. and Cholewa, M., 2018. Numerical analysis and optimization of Cu2O/TiO2, CuO/TiO2, heterojunction solar cells using SCAPS. in Journal of Physics: Conference Series. IOP Publishing.

[12] Koohestani, H. and S.K. Sadrnezhaad, 2016. Photocatalytic degradation of methyl orange and cyanide by using TiO2/CuO composite. Desalination and Water Treatment, 57(46), pp. 22029-22038.

[13] Qin, S., Xin, F., Liu, Y., Yin, X. and Ma, W., 2011. Photocatalytic reduction of CO2 in methanol to methyl formate over CuO–TiO2 composite catalysts. Journal of colloid and interface science, 356(1), pp. 257-261.

[14] Derikvandi, H. and A. Nezamzadeh-Ejhieh, 2017. Synergistic effect of pn heterojunction, supporting and zeolite nanoparticles in enhanced photocatalytic activity of NiO and SnO2. Journal of colloid and interface science, 490, pp. 314-327.

[15] Koohestani, H., Hassanabadi, M., Mansouri, H. and Pirmoradian, A., 2019. Investigation of photocatalytic performance of natural zeolite/TiO2 composites. Micro & Nano Letters, 14(6), pp. 669-673.

[16] Koohestani, H., Mansouri, H., Pirmoradian, A. and Hassanabadi, M., 2020. Investigation of Photocatalytic Efficiency of Supported CuO Nanoparticles on Natural Zeolite Particles in Photodegradation of Methyl Orange. Journal of Nanoscience and Nanotechnology, 20(9), pp. 5964-5969.

[17] Brazlauskas, M. and S. Kitrys, 2008. Synthesis and properties of CuO/Zeolite sandwich type adsorbent-catalysts. Chinese Journal of Catalysis, 29(1), pp. 25-30.

[18] Ruíz-Baltazar, A., Esparza, R., Gonzalez, M., Rosas, G. and Pérez, R., 2015. Preparation and characterization of natural zeolite modified with iron nanoparticles. Journal of Nanomaterials, 2015.

[19] Nezamzadeh-Ejhieh, A. and A. Shirzadi, 2014. Enhancement of the photocatalytic activity of ferrous oxide by doping onto the nano-clinoptilolite particles towards photodegradation of tetracycline. Chemosphere, 107, pp. 136-144.

[20] Bezrodna, T., Puchkovska, G., Shymanovska, V., Baran, J. and Ratajczak, H., 2004. IR-analysis of H-bonded H2O on the pure TiO2 surface. Journal of Molecular Structure, 700(1-3), pp. 175-181.

[21] Sacco, O., V. Vaiano, and M. Matarangolo, 2018. ZnO supported on zeolite pellets as efficient catalytic system for the removal of caffeine by adsorption and photocatalysis. Separation and Purification Technology, 193, pp. 303-310.

[22] Nezamzadeh-Ejhieh, A. and M. Karimi-Shamsabadi, 2014. Comparison of photocatalytic efficiency of supported CuO onto micro and nano particles of zeolite X in photodecolorization of Methylene blue and Methyl orange aqueous mixture. Applied Catalysis A: General, 477, pp. 83-92.

[23] Yu, D., Xu, L., Zhang, H., Li, J., Wang, W., Yang, L., Jiang, X. and Zhao, B., 2022. A new semiconductor-based SERS substrate with enhanced charge collection and improved carrier separation: CuO/TiO2 pn heterojunction. Chinese Chemical Letters, p. 107771.

 

 

[1]   Artiola, J., 2019. Industrial waste and municipal solid waste treatment and disposal, in Environmental and pollution science. Elsevie,. pp. 377-391.
[2]   Ambaye, T., Vaccari, M., van Hullebusch, E. D., Amrane, A., & Rtimi, S., 2021. Mechanisms and adsorption capacities of biochar for the removal of organic and inorganic pollutants from industrial wastewater. International Journal of Environmental Science and Technology, 18(10), pp. 3273-3294.
[3]   Wang, S. and Y. Peng, 2010. Natural zeolites as effective adsorbents in water and wastewater treatment. Chemical engineering journal, 156(1), pp. 11-24.
[4]   Metes, A., Kovac̆ević, D., Vujević, D., & Papić, S., 2004. The role of zeolites in wastewater treatment of printing inks. Water Research, 38 (14-15), pp. 3373-3381.
[5]   Korkuna, O., Leboda, R., Skubiszewska-Zie, B. J., Vrublevs’Ka, T., Gun’Ko, V. M., & Ryczkowski, J., 2006. Structural and physicochemical properties of natural zeolites: clinoptilolite and mordenite. Microporous and mesoporous materials, 87(3), pp. 243-254.
[6]   Cui, T., Liu, Z., Zheng, X., Liu, Z., Li, Y., Li, W., Wang, B., Guo, K. and Han, J., 2014. Zeolite-based CuO nanotubes catalysts: investigating the characterization, mechanism, and decolouration process of methylene blue. Journal of nanoparticle research, 16(9), pp. 1-11.
[7]   Sikhwivhilu, L.M., S. Sinha Ray, and N.J. Coville, 2009. Influence of bases on hydrothermal synthesis of titanate nanostructures. Applied Physics A, 94(4), pp. 963-973.
[8]   Liu, Z., Liu, Z., Zheng, X., Liu, Z., Li, Y., Li, W., Wang, B., Guo, K. and Han, J., 2014. Photocatalyst from one-dimensional TiO2 nanowires/synthetic zeolite composites. Materials Express, 4(6), pp. 465-474.
[9]   Koohestani, H. and S.K. Sadrnezhaad, 2016. Improvement in TiO2 photocatalytic performance by ZrO2 nanocompositing and immobilizing. Desalination and Water Treatment, 57(58), pp. 28450-28459.
[10] Subha, P., L. Vikas, and M. Jayaraj, 2018. Solution-processed CuO/TiO2 heterojunction for enhanced room temperature ethanol sensing applications. Physica Scripta, 93(5), p. 055001.
[11] Sawicka-Chudy, P., Sibiński, M., Wisz, G., Rybak-Wilusz, E. and Cholewa, M., 2018. Numerical analysis and optimization of Cu2O/TiO2, CuO/TiO2, heterojunction solar cells using SCAPS. in Journal of Physics: Conference Series. IOP Publishing.
[12] Koohestani, H. and S.K. Sadrnezhaad, 2016. Photocatalytic degradation of methyl orange and cyanide by using TiO2/CuO composite. Desalination and Water Treatment, 57(46), pp. 22029-22038.
[13] Qin, S., Xin, F., Liu, Y., Yin, X. and Ma, W., 2011. Photocatalytic reduction of CO2 in methanol to methyl formate over CuO–TiO2 composite catalysts. Journal of colloid and interface science, 356(1), pp. 257-261.
[14] Derikvandi, H. and A. Nezamzadeh-Ejhieh, 2017. Synergistic effect of pn heterojunction, supporting and zeolite nanoparticles in enhanced photocatalytic activity of NiO and SnO2. Journal of colloid and interface science, 490, pp. 314-327.
[15] Koohestani, H., Hassanabadi, M., Mansouri, H. and Pirmoradian, A., 2019. Investigation of photocatalytic performance of natural zeolite/TiO2 composites. Micro & Nano Letters, 14(6), pp. 669-673.
[16] Koohestani, H., Mansouri, H., Pirmoradian, A. and Hassanabadi, M., 2020. Investigation of Photocatalytic Efficiency of Supported CuO Nanoparticles on Natural Zeolite Particles in Photodegradation of Methyl Orange. Journal of Nanoscience and Nanotechnology, 20(9), pp. 5964-5969.
[17] Brazlauskas, M. and S. Kitrys, 2008. Synthesis and properties of CuO/Zeolite sandwich type adsorbent-catalysts. Chinese Journal of Catalysis, 29(1), pp. 25-30.
[18] Ruíz-Baltazar, A., Esparza, R., Gonzalez, M., Rosas, G. and Pérez, R., 2015. Preparation and characterization of natural zeolite modified with iron nanoparticles. Journal of Nanomaterials, 2015.
[19] Nezamzadeh-Ejhieh, A. and A. Shirzadi, 2014. Enhancement of the photocatalytic activity of ferrous oxide by doping onto the nano-clinoptilolite particles towards photodegradation of tetracycline. Chemosphere, 107, pp. 136-144.
[20] Bezrodna, T., Puchkovska, G., Shymanovska, V., Baran, J. and Ratajczak, H., 2004. IR-analysis of H-bonded H2O on the pure TiO2 surface. Journal of Molecular Structure, 700(1-3), pp. 175-181.
[21] Sacco, O., V. Vaiano, and M. Matarangolo, 2018. ZnO supported on zeolite pellets as efficient catalytic system for the removal of caffeine by adsorption and photocatalysis. Separation and Purification Technology, 193, pp. 303-310.
[22] Nezamzadeh-Ejhieh, A. and M. Karimi-Shamsabadi, 2014. Comparison of photocatalytic efficiency of supported CuO onto micro and nano particles of zeolite X in photodecolorization of Methylene blue and Methyl orange aqueous mixture. Applied Catalysis A: General, 477, pp. 83-92.
[23] Yu, D., Xu, L., Zhang, H., Li, J., Wang, W., Yang, L., Jiang, X. and Zhao, B., 2022. A new semiconductor-based SERS substrate with enhanced charge collection and improved carrier separation: CuO/TiO2 pn heterojunction. Chinese Chemical Letters, p. 107771.